Analysis and Judgment On The Cause Of Copper Wire Disconnection During Wire Drawing
1. Central burst:
The broken wire breaks from the central part of the copper wire, with a sharp cone at one end and a sharp hole at the other. The hole that burst in the center is most likely to be mistaken for the broken line of the bubble. When the wall of the hole bursting in the center is enlarged, it can be found that the material itself presents a concave-convex tearing phenomenon due to the influence of external force.
1)Types of central burst:
1.1 Central burst caused by excessive oxygen content in the copper rod (greater than 6000PPM)
1.2 Central burst caused by inclusions.
1.3 Central burst caused by poor wire drawing machine (such as inappropriate eye mold angle)
2)The formation process of the central burst
Observing the metallographic photo of the longitudinal section of the central burst fracture line, we found that the cuprous oxide particles that were originally arranged in order were distorted and irregular due to the influence of stress. The formation process of the fracture line was observed from the metallographic diagram. (As shown in the figure; the cuprous oxide particles have been obviously distorted and concentrated, and tiny cracks have occurred, and the wire has not been broken at this time), If this phenomenon is caused by using rod breakdown machine to draw the wire, although there is sufficient strength to maintain the continuous wire, as long as external force is applied during the subsequent intermediate wire drawing process, the wire will inevitably be broken. There is bound to be a problem when use the fine wire drawing machine to draw the wire. (When a wire breakage occurs, the drawn copper wire is hard and brittle, and breaks when it is bent, which is often mistaken for poor copper quality.)
3)Prevention of Central Burst
Due to the relatively stable quality of continuous casting and tying copper rods, there are few other reasons for wire breakage, so the prevention of central bursting is particularly important. Prevention methods:
3.1 Regularly check the deformation angle of the eye mold, if the wear is too large, it should be replaced in time.
3.2 Regularly check the concentration, temperature, PH value and electrical conductivity of the drawing liquid, and add or replace the drawing oil in time.
3.3 Check the tower wheel of the wire drawing machine and replace it in time when it is seriously worn.
2. Bubble disconnection (mainly caused by copper)
The section of this broken line is hole-shaped, and the surface of the hole is very smooth, without bulging or cracking.
The reason for the formation of bubble breakage is the improper control of hydrogen during casting, and the shrinkage cavity caused by poor cooling. If the hole is small, it may be closed in the subsequent hot working process. If the hole is large, it cannot be closed, resulting in a new line of bubbles.
3. Inclusion disconnection (mainly due to copper)
Inclusion disconnection is a common type of disconnection, which can be divided into two categories in terms of appearance, one is the disconnection with the presence of inclusions, and the other is the disconnection with missing inclusions.
4. Copper thorns or splinter (mainly due to copper)
The occurrence of copper thorns is similar to that of inclusions, which are generated during rolling or casting, so they can be divided into two types: cast (CAST-INSLIVER) and rolled (ROLLED-INSLIVER). The oxygen content in the copper water is too high; the copper thorns are formed from the extension process, the trimmer is not adjusted properly, or the gap between the tie wheels is not adjusted properly, resulting in scratches, etc.
Generally speaking, copper thorns or long splits are related to cuprous oxide particles that occur during casting or drawing, because the presence of cuprous oxide prevents the copper rod from closing the cracks during processing, so the copper wire surface produces thorns after stretching. Or long slivers, causing wire breakage in severe cases.
5. Tension disconnection
Tension wire breakage is a common kind of wire breakage in the wire drawing process. The wire breakage is characterized by the shape of a cone or a pointed cone. The wire breakage is caused by the tensile force being greater than the tensile strength of the copper wire itself.
Causes: When operating copper wire drawing machine,the lubrication is poor and improper eye mold angle, accumulation of copper powder in front of the eye mold, excessive surface reduction rate and improper speed matching may cause tension disconnection.
6. Copper powder disconnection
There is a considerable amount of copper powder in the drawing lubricant. When drawing, the copper powder will accumulate at the corner of the eye mold, so that the copper wire will be clamped in the eye mold and cause wire breakage. In addition, copper thorns peeling off and accumulating before the eye mold will also cause breakage wire.
7. Connector disconnection
The shape of the connector disconnection can be divided into four categories: fish mouth-shaped disconnection, and the other three are flat-headed, oblique-edged, and thorn-shaped.
The biggest reason for the disconnection of the joint is that the cuprous oxide particles are too concentrated in the connection part, or the temperature is too high during the wiring, which causes the growth of the grains. In addition, the lace is not cleaned cleanly after welding, which will also cause the wire to break.